Categories
-
Pharmaceutical Intermediates
-
Active Pharmaceutical Ingredients
-
Food Additives
- Industrial Coatings
- Agrochemicals
- Dyes and Pigments
- Surfactant
- Flavors and Fragrances
- Chemical Reagents
- Catalyst and Auxiliary
- Natural Products
- Inorganic Chemistry
-
Organic Chemistry
-
Biochemical Engineering
- Analytical Chemistry
-
Cosmetic Ingredient
- Water Treatment Chemical
-
Pharmaceutical Intermediates
Promotion
ECHEMI Mall
Wholesale
Weekly Price
Exhibition
News
-
Trade Service
The baking temperature is too low or the time is too short
White powder will produce a color that is white and not yellow enough
Increased powder gloss
Impact, bending, adhesion, surface hardness of the coating film,
Poor chemical resistance and other performance
The difference between gas stove and diesel stove and electric stove
When the gas is baked, it is white, and the light gray powder is easy to use
The powder is yellowish and darker
Diesel furnace and electric furnace are relatively close to the laboratory effect
Common symptoms
The appearance of the customer sprayed product has particles
v cause
? Coating film is too thin
? The workpiece is not thoroughly cleaned
? Poor spraying environment
?The spraying operator wears fiber clothing or there are fibers on the surface of the workpiece
? There is no oil baffle on the suspension chain
The drying tunnel is not cleaned regularly or incorrectly
?The powder itself has particles
Judgment method
v Observe on-site product quality
v Understand the size, shape, quantity and distribution of shrinkage holes
v Pass the comparison test
There is shrinkage on the surface of the sprayed product of the customer
cause:
The substrate or powder is contaminated, which makes the local surface tension of the powder inconsistent
? Incomplete treatment before painting, including insufficient oil removal
? Environmental factors, such as suspension chain lubricating oil, compressed air oil
The water is not separated in time, and the drying effect is not good
? The quality of the powder itself
The powder penetration is poor and cannot reach the dead corner of the workpiece
cause
? Poor grounding between the equipment and the workpiece
The set voltage of the spray gun is too high, the powder
The powder output is too large or too small
The distance between the spray gun and the workpiece is too far or too close
The proportion of recycled powder used is too large
?Powder cause
Poor leveling and obvious orange peel
cause
? Coating is too thin
?The curing heating speed is too slow or the curing temperature and time are not enough
?Powder cause
There are pinholes on the coating surface
cause
? The coating is too thick
?The spray gun voltage setting is too high
? Poor grounding of spray equipment
The distance between the spray gun and the workpiece is too close
The powder is contaminated or damp, and the compressed air has more moisture
?The reason for the base material of the customer's workpiece
?Powder cause
(Source: Global Coatings Network) (For more information, please log in: Global Coatings Network http:// )